Alphasol S100

 

GENERAL

Typical properties

Active content, (%)

93 min.

Pour point, (¡É)

-4

Cloud point, (¡É)

N. A.

Kinematic viscosity (40¡É, cst)

60 ~ 110

Surface tension (20% dyne /§¯)

31 ~ 33

Whiteness (5% emulsion)

85 ~ 95

Emulsion stability

No separate in soft water

No separate in hard water

 

Results

 Test  item

Typical results

Remarks

Absorption, (%)

9.0 min.

 

Scouring(Degumming) loss, (%)

15 ~ 30

 

Tenacity, (g/d)

3.0 min.

 

Elongation, (%)

18.0 min.

 

Modulus, (g/d)

90.0 min.

 

Loss of raw silk after treatment, (wt%)

8.0 max.

 

Remained fat and wax content, (g/kg)

2.0 ~ 3.0

Raw silk

~0

Degummed silk

 

Yarn cutting during reeling, (Number/Time)

0.3 max.

 

Yarn rupture during reeling, (Number/Yard)

0.2 max.

 

Yarn cutting during twisting, (Number/Time)

0.2 max.

800(T/M)

0.4 max.

2000(T/M)

Yarn cutting during weaving, (Number/Yard)

1 max.

800(T/M)

2 max.

2000(T/M)

HOW TO USE

 * Recommended dipping recipe: 

       -     1~3 % of weight of Raw silk

-     120kgs of silk

-     1~4Kgs of S-100

-     Applicable amount of water(thoroughly submerged)

-     Degree of degumming  is varying with the concentration of Alphasol and  dipping time. //Dipping temperature : 40~50¡É//Dipping time : 10~15  hours//Drying : The ambient is desirable.

-      In case of drying room,  35¡É to 45¡É is proper.

PACKAGING

16kgs / PE Pail,

160 kgs / HDPE Drum